Wet filament: how to spot it, dry it and keep it dry
Wet filament shows up as popping at the nozzle, bubbles in the extruded plastic, more stringing and a rough surface. Dry the spool at the temperature and time its own manufacturer states, then seal it in an airtight container with desiccant straight away. The figures differ between manufacturers, so we list each one separately on this page.
Signs of wet filament: listen at the nozzle, look at the surface
Bambu Lab explains that moisture in the filament turns to vapour as soon as it meets the hot nozzle, so the melt expands and flows faster than normal. In severe cases the nozzle clogs or the filament stops feeding.
Stringing alone does not prove a spool is wet. Prusa notes that some filaments are naturally stringy, so compare against your earlier prints. UltiMaker warns that at lower moisture levels the effect on the part can be large even though nothing is visible yet.
- Popping sounds at the nozzle and bubbles in the extruded plastic. Bambu Lab and Anycubic both list this, and Polymaker says to dry PETG if you hear popping or cracking while it extrudes.
- More stringing and oozing. Bambu Lab says obvious stringing on a PETG print indicates the filament is damp.
- A rough surface, holes or blobs. Prusa says the first sign is usually poor surface quality.
- Poor layer adhesion, as listed by Bambu Lab and Prusa. Bambu Lab adds reduced structural strength.
- Bubbling and smoke during extrusion, as listed by Prusa.
- Damp PETG may stick to the heated bed too strongly, according to Elegoo.
- Damp PVA turns soft and sticky. Bambu Lab says it is then unsuitable for the AMS and AMS lite and causes loading failures and nozzle clogs.
Which materials absorb moisture fast, and which must be dried first
Manufacturers do not group materials identically. The names that recur across several guides are PVA, TPU and nylon.
- Bambu Lab’s table puts PLA Wood, TPU, PC, PVA, PA6-CF, PAHT-CF, PET-CF, PPA-CF and PPS-CF under drying required before use, and PLA Basic, PLA Matte, PLA Silk, PETG, ABS and ASA under drying recommended.
- Bambu Lab says PLA has low hygroscopicity and needs drying less often than PETG or nylon, and calls PETG highly hygroscopic.
- Prusa lists polyamide (nylon), polypropylene, PVA and BVOH as highly hygroscopic, and says polyamide, PVA and TPU need drying more often than PLA.
- UltiMaker names Nylon, Nylon CF Slide, PVA and TPU95A as moisture-sensitive.
- Elegoo marks TPU and PC as drying required before use, and says PETG can absorb moisture quickly.
- Bambu Lab says freshly dried PVA left in a room at about 55% relative humidity gets damp again in about 1 to 3 hours.
PLA and PETG drying temperature and time, by manufacturer
The manufacturers’ figures do not match, and we do not average them. Check the label or guide for the brand of filament you are using first. Elegoo sets the same order: the parameters from the filament manufacturer first, then the preset on the dryer. Bambu Lab says its table is based on tests with Bambu Lab filaments, so values may vary with third-party filament.
One manufacturer can publish more than one set of figures. Bambu Lab’s PLA page gives 55°C for 8 hours in the AMS HT or AMS 2 Pro for PLA Silk, Wood and Aero, while its main drying table in this list gives PLA Basic 45°C for 12 hours.
- PLA, Bambu Lab main table (PLA Basic and Matte): 45°C for 12 hours in the AMS 2 Pro or AMS HT, 55°C for 12 hours in the AMS 3P or AMS 3H, 50°C for 8 hours in a convection oven, 60-70°C for 12 hours on the heated bed.
- PLA, Prusa table (PLA and rPLA): 45°C for 6 hours.
- PLA, UltiMaker table (PLA and Tough PLA): 40°C in a PrintDry dryer or 50°C on the build plate, for 4-8 hours.
- PLA, Elegoo guide: 55 ± 5°C for 6 hours. The PLA preset on the Elegoo H1 HT dryer is 55°C for 8 hours.
- PETG, Bambu Lab main table (PETG and PETG-CF): 65°C for 8 hours in the AMS 2 Pro, AMS HT or AMS 3H, 65°C for 12 hours in the AMS 3P, 60-65°C for 8 hours in a convection oven, 75-85°C for 12 hours on the heated bed.
- PETG, Prusa table (all versions): 55°C for 6 hours.
- PETG, UltiMaker table (PETG and CPE): 65°C for 4-8 hours in a PrintDry dryer, or 70°C for 10-20 hours on the build plate.
- PETG, Polymaker PETG product page: 60°C for 6 hours.
- PETG, Elegoo guide: 60 ± 5°C for 8-10 hours. The PETG preset on the H1 HT is 65°C for 8 hours.
TPU and PVA drying temperature and time, by manufacturer
The figures for these two are far apart. Bambu Lab dries PVA at 85°C in the AMS HT, while UltiMaker dries PVA at 50°C in a dryer. Do not carry one brand’s figure over to another brand’s filament.
ABS, ASA, PC and nylon have their own figures. For example, Bambu Lab’s main table gives ABS and ASA 80°C for 8 hours in the AMS HT, and Prusa gives ASA 80°C for 4 hours. The full tables are on the manufacturer pages in the source list.
- TPU, Bambu Lab main table (TPU 85A and 90A): 75°C for 18 hours in the AMS HT, 70°C for 8 hours in a convection oven, 90°C for 16 hours on the heated bed. The AMS 3P and AMS 3H use 75°C for 18 hours when idle and 65°C for 18 hours when printing while drying.
- TPU in the AMS 2 Pro: Bambu Lab’s table gives 65°C for 12 hours with a warning mark that this method may not fully dry the filament.
- TPU, Prusa table: 60°C for 4-6 hours.
- TPU, UltiMaker table (TPU95A): 70°C for 4-16 hours in a PrintDry dryer, or 70°C for 10-20 hours on the build plate.
- TPU, Polymaker PolyFlex TPU95 technical data sheet: 70°C for 8 hours.
- TPU, Elegoo guide: 70 ± 5°C for 6-10 hours. The TPU preset on the H1 HT is 70°C for 8 hours.
- TPU, Anycubic recommendation: 50-55°C for 4-6 hours.
- PVA, Bambu Lab main table: 85°C for 18 hours in the AMS HT, 75-85°C for 8-12 hours in a convection oven, 90-100°C for 12 hours on the heated bed. The AMS 2 Pro at 65°C for 12 hours carries the same warning mark as TPU.
- PVA, UltiMaker table: 50°C in a PrintDry dryer or 55°C on the build plate, for 10-20 hours.
- PVA, Elegoo H1 HT dryer preset: 80°C for 8 hours.
What to dry it with: a filament dryer, an AMS, the heated bed or an oven
UltiMaker puts a dedicated drying device first and the heated build plate second. Humidity is not controlled on a build plate, so it takes longer and needs a higher temperature.
A storage box with desiccant is not a dryer. UltiMaker says storing material with silica desiccant in the packaging does not dry it, and Prusa says the same of its own USS Drybox. Filament that is already damp has to be dried first.
- Filament dryer: Prusa says to check that the box reaches the temperature the material needs. Elegoo says to keep the H1 HT lid closed, because opening it often may lengthen the drying time.
- Bambu Lab’s drying-capable AMS units: the maximum is 65°C for the AMS 2 Pro, 75°C for the AMS 3P with the Filament Dryer Module, and 85°C for the AMS HT and AMS 3H. Bambu Lab says the AMS 2 Pro suits filament with a drying temperature no higher than 65°C, such as PLA and PETG.
- Heated bed: Bambu Lab allows this only on an enclosed printer. The P1P, A1, A2L and A1 mini are open-frame and cannot dry filament this way. Unload the filament from the toolhead first, cover the spool with the filament’s original cardboard box, and flip the spool every 6 hours wearing gloves.
- Convection oven: Bambu Lab counts it as one of its three methods, but Prusa warns that home ovens are imprecise and many cannot go low enough. Use an external thermometer. Temperature swings can damage filament, especially PLA.
- Food dehydrator: Prusa says it has to be modified to fit a spool and usually reaches only low temperatures.
Before you start: deformed spools and filament that sticks together
The heat that dries the filament can also soften the spool and the filament itself. Check these four points before you press start.
- Check what the spool can take. Bambu Lab classes its own spools as low-temperature (up to 70°C) and high-temperature (up to 90°C), and warns that third-party or 3D-printed spools may not withstand high temperatures. UltiMaker says its spools can soften at around 80°C, so a full spool must be dried below that.
- Do not go above the recommended temperature. Prusa warns the filament will soften and stick together, and says to stick to the recommended times to avoid overdrying.
- Do not dry low-temperature and high-temperature filament together in an AMS. Bambu Lab says PLA and TPU must be removed from the AMS before drying ABS or PETG, or the filament may soften and deform.
- In an AMS, use rotating drying. Bambu Lab says static drying is not suitable for PLA, PVA and TPU, because the filament may stick together, expand or deform.
How to store filament after drying so it stays dry
Bambu Lab says to wait 5-10 minutes until the spool is no longer hot, then store it immediately in a sealed container or an AMS with effective desiccant, and use it as soon as possible.
Bambu Lab says PLA can be stored normally at 50%-60% ambient humidity, but PETG absorbs moisture at that same level, and absorbs more the longer it is stored and the higher the humidity.
- Keep the spool in its original plastic packaging with the desiccant and clip the opening shut, or use a vacuum bag with desiccant, as Elegoo describes.
- Store filament in a closed space or box with desiccant. Where space is limited, Prusa says to give priority to the more hygroscopic materials.
- Keep it in a cool, dry place, out of direct sunlight and away from heat sources, as Bambu Lab advises.
- If your box has a hygrometer, Prusa’s maximum recommended values for its USS Drybox are below 30% RH for PLA and below 20% RH for PETG, TPU and PVA.
- PVA needs stricter storage. Bambu Lab says to keep it below 20% RH and to use calcium chloride desiccant, because silica gel cannot keep PVA dry for long. Do not put calcium chloride in the Elegoo H1 HT dryer: Elegoo warns it may produce liquid and damage the device.
- For leftover TPU, Anycubic says to seal it promptly and label the hardness, colour and date opened.
- Elegoo says leaving filament in the H1 HT dryer is fine for short-term storage. For long-term storage, move it to a moisture-resistant bag, a vacuum bag or another sealed container with desiccant.
Frequently asked questions
Does PLA need drying before printing?
Not every time. Bambu Lab says PLA has low hygroscopicity and lists PLA Basic under drying recommended, not required. PLA Wood is the exception and must be dried before use. If stringing or bubbles appear, dry the spool at the figure for the brand you are using.
Does a brand-new spool need drying?
Elegoo says newly opened filament is typically dry, but it needs drying after several days or months in humid conditions. Bambu Lab and Elegoo both mark TPU and PC as materials that must be dried before use.
Can I dry filament in a kitchen oven?
Yes, with care over the temperature. Bambu Lab counts a convection oven as one of its three drying methods. Prusa warns that home ovens are imprecise, many cannot go low enough, and temperature swings can damage filament, especially PLA. Check the real temperature with an external thermometer every time.
Will desiccant in a storage box dry a damp spool?
No. UltiMaker says storing material with silica desiccant does not dry it, and that dry boxes only keep dry material dry. Prusa says its USS Drybox does not dry filament either. A damp spool has to be dried before it goes into storage.
Can the AMS 2 Pro dry every filament?
No. The AMS 2 Pro dries at up to 65°C. Bambu Lab says it suits filament such as PLA and PETG, and its table marks TPU, PVA, ABS, ASA and PC with a warning that the AMS 2 Pro may not fully dry them. The AMS HT and AMS 3H reach 85°C.
How do I know the spool is dry enough?
For its H1 HT dryer, Elegoo gives three checks: the recommended time has finished, the chamber humidity has dropped significantly and stabilised, and symptoms such as stringing or surface pitting are clearly reduced on the next print. For moisture-sensitive filament that holds a lot of moisture, UltiMaker says to dry overnight, for 10-20 hours.
Manufacturer sources
- Bambu Lab Wiki — Filament Drying Recommendations
- Bambu Lab Wiki — PLA Usage Guide
- Bambu Lab Wiki — PETG Usage Guide
- Bambu Lab Wiki — PVA Printing Guide
- Prusa Knowledge Base — Drying filament
- Prusa Knowledge Base — Prusa USS Drybox
- UltiMaker Support — How to dry Ultimaker materials?
- Polymaker Wiki — Polymaker™ PETG
- Polymaker Wiki — PolyFlex™ TPU95
- Elegoo Wiki — Guide to FDM Printing Filament
- Elegoo Wiki — H1 HT FAQ
- Anycubic Wiki — TPU printing